We are using wet-mix shotcrete for culvert linings, with an existing corrugated steel plate pipe stream culvert. The pipe is 96 in. (2438 mm) long and deteriorated. There is a water diversion, but there is a pressure gradient forcing water through the voids. Any ideas on leak repair procedures?

Installing a shotcrete lining requires a somewhat dry substrate and certainly is not compatible with running water. The water needs to be blocked or diverted.
A means of blocking the inflow is to inject a swellable urethane grout through the openings in the existing pipe. The grout, if done properly, will expand upon contact with water and seal the outside of the pipe. Another means of diverting the water is to install drainage material over the inflowing area to collect the water and remove it from the pipe. The shotcrete can then be applied over the drainage material.

I am an engineering technologist working on a landslide project where shotcrete had been applied to stabilize the sandstone head scarp at the crest of the slope. The shotcrete was applied in 1998. After a recent inspection, it was noted that the surface of the shotcrete had some cracking in some sections. How can this be repaired? Can the cracks simply be filled with a grout/mortar mixture of some sort or do the cracked sections have to be removed entirely and shotcrete be reapplied?

Shotcrete can and has been used to overlay previously installed shotcrete or concrete that has cracked over time. It would be advisable that you engage an engineer knowledgeable in geotechnical engineering and concrete properties to formalize a solution. It is important that the cause of the cracks be determined and adequate reinforcing be designed to ensure that the cracks do not propagate through the overlaid shotcrete.

We have a 17 mile (28 km) long TBM tunnel for water that will drive our underground powerhouse. Is there a recommended shotcrete surface texture we could use? Our contractor is using 0.31 in. (8 mm) aggregate, but they are getting an undulating surface. Can you provide some clarity as to what we should ask our contractor to try and achieve?

Shotcrete can be applied with many different textures. The nozzle finish shown is very rough, even for a natural gun finish. Nozzle finishes can be done smoother than this. Another technique would be to use a broom to make it smoother after it is shot. Other finishes include wood float, rubber or sponge float, broom, and smooth trowel finishes. There are many examples of finishes shown in articles in Shotcrete magazine.

I am an engineer working on a project involving shotcrete and earthwork. The shotcrete that was placed has some expansion cracks, which we expected. I would like to know the best way to repair them. Is there some type of waterproof coating/grout that can be applied between the cracks? Part of the cracks will be continuously under water. The shotcrete is the surfacing material for a diversion ditch at a mine, and we need to recommend some remediation solutions to our client.

There are many products in the marketplace for repairing cracks. Because shotcrete is simply a method for placing concrete, any method for concrete crack repair would be applicable. It would be wise to use a product that filled the cracks and is able to tolerate thermal movement in the future (not a brittle product). Many injectable polyurethane grouts can accomplish this. Surface-applied coatings would need an adequate thickness and elasticity to tolerate moving cracks. We suggest that you contact one of our corporate members who is familiar with your area and get their specific advice. Please refer to “ASA’s Buyers Guide”.

I am a structural engineer working on underground structures such as tunnels and caverns. I would like to know the permissible shear strength of shotcrete to be taken for M30 Grade SFRS (M30 = 30 MPa [4350 psi] at 28 days). I would like to know more about its other properties, as well.

Shotcrete is simply a placing method for concrete. Thus, the in-place material properties are essentially the same as cast concrete. A specific value for the shear is beyond the scope of our Association because many design and material properties can affect the shear capacity. We would suggest you engage a Professional Engineer who specializes in Underground Shotcrete. You should consult our Buyers Guide to find such a consultant. ACI 506R-05, “Guide to Shotcrete”, would be a helpful primer to learn more about shotcrete.

I am evaluating a community in central Colorado that contains shotcrete slope reinforcement ranging from 14 to 44 ft (4 to 13 m) in height. Assuming the installation met all required guidelines, what should I anticipate as a useful life for this product?

Shotcrete is a method of placing concrete and properly placed shotcrete should have a service life similar to cast concrete. Generally, concrete structures in normal environmental exposures are expected to have service lives from 50 to 100 years. With particular attention to materials and construction methods, some concrete structures, such as the new San Francisco Bay Bridge, have been designed for a service life up to 150 years. The first step in achieving a long-lasting, high-quality installation is to engage a highly qualified and experienced shotcrete contractor. There are many other factors that influence service life, including using the right mixture design for the anticipated exposure conditions.

I am a Civil Engineer working on a hydropower project. Is it possible to place shotcrete at a thickness of 24 in. (600 mm) inside a tunnel that will be used as a water tunnel to generate power?

Yes, it is possible to shoot 24 in. (600 mm) thick tunnel linings. There are various ways of doing this, depending on the reinforcing steel configuration. One method we have successfully used for shooting tunnel linings this thick with a double mat of reinforcing bar (1 in. [20 mm] diameter bars at 6 in. [150 mm] on center, vertically and horizontally) is to bench gun shoot the walls up to the spring line with a wet-mix silica-fume-modified shotcrete (without accelerator) and then ribbon-shoot (2 ft [0.5 m] wide strips) overhead using the same mixture but with the option of using an alkali-free accelerator added at the nozzle.
If the shotcrete requires a smooth finish (equivalent to a cast-in-place concrete finish), then the initial shotcrete is shot to within about 1 in. (30 mm) of the final shotcrete thickness and allowed to set and harden. Following that, a final non-accelerated finish coat can be applied that can be trimmed to shooting wires with a cutting rod, closed up with a darby, and then trowelled with either a magnesium or steel trowel, depending on the required finished surface texture.
Such work can be done with a remote-control manipulator arm (robot) or, for more precision, with hand nozzling out of a basket on a manlift (provided the tunnel floor is sufficiently smooth for operation of a manlift). The bottom line: hire a contractor who has experience in conducting such work.

We are working on a geotechnical project in the northwest to repair an existing rockery retaining wall. The wall is around 750 ft (229 m) in length and up to 12 ft (4 m) in height. The issue is that some of the basalt boulders within the wall are weathered soft and falling apart. The total weathered rocks that are falling apart comprise approximately 7% of the wall. Can we use shotcrete on the weathered rocks to give them more stability as a repair process? If not, is there a process we can use with shotcrete to repair the wall without having to rebuild the entire wall?

Shotcrete has been used in the Northwest to strengthen and overlay existing rockery walls. The need to remove the weathered material is dependent upon the need for the overlay to bond with the existing wall, which is an engineering issue and not a shotcrete issue. Shotcrete can and is shot successfully against soil and other weathered surfaces.